1. Materials at a Glance
A. Material Summary
This is a quick reference to help operators choose the right material efficiently.
Covered grades: WC, SKH51, SKD11, SUS440C, 420J2, SK5, S45C (AISI 1045), SCM440 (AISI 4140)
| Grade | Recommended Hardness (HRC/HRA/HV) | Key Traits | Typical Applications | Alternatives / Options |
| WC (WC–Co) | HRA 89–92 (HV 1600–1800) | Extreme wear resistance / very high hardness / chipping risk under impact | Film & foil slitting; glass-fiber & filled plastics | If impact is high → consider SKH51 / for anti-stick & contamination-sensitive lines → DLC (optional) |
| SKH51 (HSS/M2) | HRC 60–63 | Balanced heat & wear performance / general-purpose / good impact tolerance | Granulator & recycling; general slitting; straight/shear cutting; multi-purpose cutting | Longer life → TiN/TiAlN / severe abrasion or difficult-to-cut materials → consider WC |
| SKD11 (D2) | HRC 58–61 | Stable wear resistance / secondary hardening / dimensional stability management is important | Metal shearing; rubber/tire cutting; conditional granulator use | Stability & life ↑ → cryo (recommended) / corrosion- or cleaning-heavy environments → 440C |
| SUS440C | HRC 56–60 | Corrosion resistance / hygiene / finishing & cleaning are critical | Food & wet lines; frequent cleaning; tape/film (anti-stick & contamination control) | Anti-stick ↑ → DLC / higher impact requirement → 420J2 (lower hardness) |
| 420J2 | HRC 48–52 | Corrosion resistance / machinability / economical | Low-load cutting; entry-level solutions for wet environments | Higher hardness & life → upgrade to 440C |
| SK5 | HRC 58–62* | Cost-effective / sharp / easy maintenance | Paper & thin sheet; low-difficulty cutting; general straight knives | Longer life → upgrade to SKH51 / for corrosion environments → stainless options |
| S45C (AISI 1045) | HRC 18–25 (Q&T ~25–35) | Cost-effective / good machinability / general structural steel | Base plates, fixtures/jigs, spacers, general holders/bodies (medium duty) | Higher strength/toughness/fatigue margin → SCM440 / higher surface wear resistance → induction/case hardening (case-dependent) |
| SCM440 (AISI 4140) | HRC 30–45 (or nitrided) | High toughness & impact resistance / structural base material | Knife holders/bodies; shafts/housings; heavy-duty fixtures | Surface hardness ↑ → nitriding / coating / plating (often combined) |
* SK5 target hardness can vary depending on geometry, quench method (oil/water), and distortion control.
Note: S45C/SCM440 are recommended for holders/fixtures/structural parts rather than cutting edges.
B. Key Trade-off: Hardness (HRC) vs Toughness
Understanding the trade-off between wear resistance and impact resistance (toughness) helps you select the right grade.
| Grade | Recommended Hardness | Relative Toughness | Selection Notes |
| WC (WC–Co) | HRA 89–92 | Lowest (brittle) | Avoid impact/foreign objects. Best wear resistance. |
| SKD11 (D2) | 58–61 | Medium | Balanced wear & toughness. For high impact, consider SKH51. |
| SKH51 (HSS/M2) | 60–63 | High | Better for repeated impact/high speed/heat-affected cutting. |
| SUS440C | 56–60 | Low–Medium | Best for corrosion/hygiene. If impact is higher, 420J2 is an option (lower hardness). |
| 420J2 | 48–52 | Medium–High (relative) | Prioritizes corrosion resistance & cost; limited under high wear/high load. |
| S45C (1045) | 18–25 (Q&T 25–35) | High–Highest (structural) | Great for general holders/jigs. For higher impact/fatigue margin, SCM440 is preferred. |
| SCM440 (4140) | 30–45 | Highest (structural) | Ideal for holders/structural parts. Not recommended as a cutting-edge material. |
C. Typical Chemistry (wt%)
The ranges below are typical values. Actual chemistry should follow the applicable standard, supplier specification, and mill test certificate (MTC).
| Grade | C | Cr | Mo | W | V | Co | Ni | Si | Mn | Notes |
| WC–Co | 6–12 |
|
| WC-based with Co binder (toughness control) |
|
|
|
|
|
|
| SKH51 (M2) | 0.78–0.88 | 3.75–4.50 | 4.50–5.50 | 5.50–6.70 | 1.75–2.20 | ≤0.30 | ≤0.45 | ≤0.40 |
| High-speed tool steel (heat & wear resistance) |
| SKD11 (D2) | 1.40–1.60 | 11.0–13.0 | 0.70–1.20 | 0.70–1.00 | ≤0.30 | ≤0.60 | ≤0.60 |
|
| High-C high-Cr air-hardening steel |
| SUS440C | 0.95–1.20 | 16.0–18.0 | 0.40–0.75 | ≤0.50 | ≤1.00 | ≤1.00 |
|
|
| Martensitic stainless steel |
| 420J2 | 0.26–0.36 | 12.0–14.0 | ≤0.50 | ≤1.00 | ≤1.00 |
|
|
|
| Low-C series; machinability & corrosion resistance |
| SK5 | 0.80–0.90 | (residual) | (residual) | (residual) | (residual) | (residual) | 0.15–0.35 | 0.30–0.50 |
| Carbon tool steel, economical |
| S45C (1045) | 0.42–0.48 | ≤0.30 | ≤0.10 | ≤0.30 |
|
| 0.15–0.35 | 0.60–0.90 |
| Medium-carbon steel (general structural) |
| SCM440 (4140) | 0.38–0.43 | 0.80–1.10 | 0.15–0.25 | ≤0.25 |
|
| 0.15–0.35 | 0.75–1.00 |
| Cr-Mo alloy steel (toughness & impact resistance) |
2. Heat Treatment & Coating
A. Recommended Heat-Treat Summary
The following are general guidelines. Actual parameters should be adjusted based on section thickness, geometry, equipment (vacuum/gas/salt/oil), and target microstructure.
Soak time is shown as “after equalization” (when the entire section has reached the target temperature).
| Grade | Austenitize (°C) | Hold (after equalization) | Quench | Temper (°C / cycles) | Cryo | Target Hardness |
| SKH51 (M2) | 1210–1230 | 5–15 min | Gas/Oil | 540–560 ×3 (≥1 h each) | Optional | HRC 60–63 |
| SKD11 (D2) | 1010–1040 | 10–30 min | Air/Gas/Oil (case-dependent) | 510–530 ×2–3 | Recommended (-80 to -196°C) | HRC 58–61 |
| SUS440C | 1040–1070 | 15–30 min | Air/Gas/Oil (case-dependent) | 150–200 ×2 | Optional | HRC 56–60 |
| 420J2 | 980–1050 | 10–20 min | Air/Oil | 180–250 ×1–2 | Optional | HRC 48–52 |
| SK5 | 780–820 | 5–15 min (thin sections) | Oil/Water (geometry dependent) | 150–220 ×1–2 | Optional | HRC 58–62 |
| S45C (1045) | 820–860 (case-dependent) | 20–40 min | Oil/Water (geometry dependent) | 500–650 ×1 | - | HRC 18–25 (or Q&T 25–35) |
| SCM440 (4140) | 830–860 | 20–40 min | Oil | 500–650 ×1–2 | - | HRC 30–45 (or nitrided) |
| WC–Co | Sintered product | - | - | - | - | HRA 89–92 |
440C tempering note (corrosion resistance):
To maintain corrosion resistance, low-temperature tempering at 150–200°C is recommended. In general, the ~425–565°C range has a higher risk of corrosion resistance loss (sensitization/carbide precipitation), so it is safer to avoid unless specifically required.
B. Coating Selection Guide
| Substrate | Recommended Coating | Expected Benefit | Recommended Lines / Applications | Notes |
| SKH51 | TiN / TiAlN | Wear & heat resistance / oxidation resistance | High-speed slitting, dry cutting | Minimize edge dulling (thin film, low-temp PVD preferred) |
| SKD11 | TiN | Lower friction, longer life | Metal shearing, conditional granulator use | Coat after stabilized HT; manage regrinding interval |
| SUS440C | DLC | Anti-stick, low friction, cleanliness | Food, tape/film; wet lines; frequent cleaning | Avoid edge overheating (low-temp process); use non-adhesive property |
| 420J2 | DLC (light) | Anti-stick, cleanliness | Low-load cutting; hygienic processes | Hardness limit → for overload processes, upgrade to 440C |
| WC–Co | Usually none / DLC optional | Already very hard; friction/contamination reduction | Sticky film; contamination-sensitive lines | DLC only for special cases |
| S45C / SCM440 | Nitriding / surface hardening / coating (optional) | Hard surface layer & wear resistance | Holders/contact surfaces | Structural parts, not cutting edges |
3. Specs & Tolerances
A. Standard Dimensions
A-1. Circular Slitter
| OD (mm) | ID (mm) | Thickness t (mm) | Recommended Max Line Speed (example) | Notes |
| 80–400 | 8–100 | 0.05–10.0 | ≤2,000 m/min (case-dependent) | Keyway/pin holes on request |
| 400–800 | 20–150 | 0.10–15.0 | ≤1,500 m/min (case-dependent) | On request |
| 800–1,200 | 25–200 | 0.30–20.0 | Line/material dependent | On request |
A-2. Straight / Shear Blade
| Length L (mm) | Width W (mm) | Thickness t (mm) | Edge Angle (example) | Notes |
| 50–2,000 | 5–300 | 0.30–80.0 | 15–35° (case-dependent) | Mounting holes on request |
B. Tolerance Classes
| Item | Standard | High Precision | Measurement / Notes |
| Thickness tolerance | ±0.01–0.02 mm | ±0.005–0.010 mm | Multi-point measurement across full area |
| Concentricity | ≤0.02–0.03 mm | ≤0.01–0.02 mm | Circular: based on OD–ID |
| Run-out | ≤0.02–0.03 mm | ≤0.01–0.02 mm | Recommend tighter for high-speed rotation |
| Flatness | ≤0.02 mm/300 mm | ≤0.01 mm/300 mm | Common for circular & straight |
| Parallelism | ≤0.02 mm | ≤0.01 mm | Straight blades |
| Straightness | ≤0.03 mm/1,000 mm | ≤0.02 mm/1,000 mm | Long blades |
| Bore tolerance | H7–H8 | H6–H7 | Fit to mounting standard |
| Keyway/pin-hole location | ±0.05 mm | ±0.02–0.03 mm | Includes pitch/phase |
| Balancing | G6.3 | G2.5 | ISO 21940; tighten for high-speed |
Balancing note (ISO 21940): G2.5 is advantageous for vibration control on high-speed/precision lines, but the required grade depends on speed, holder design, and assembly condition.
C. Surface & Edge Finish
| Item | Recommended | Process/Condition | Notes |
| Surface roughness Ra | 0.1–0.3 μm (high speed) / 0.4–0.8 μm (general) | Grinding finish | Balance between quality & life |
| Corner radius | R 0.02–0.05 mm | Edge protection | Prevent micro-chipping |
| Micro-rounding | 5–15 μm (by use) | Edge stabilization | Avoid excessive rounding |
| Burr control | No visible burr | Final deburring | Inspect both sides |
| Cleaning | Cleaned if required | Food/film | Prevent contamination/adhesion |
4. Reference Conditions & Performance Modeling
Disclaimer: This document is an engineering guideline provided by HD KNIFE and should not be treated as guaranteed performance. Actual tool life varies significantly depending on line conditions (gap, speed, lubrication, material, setup accuracy, foreign objects, etc.). Sample evaluation is recommended for first-time applications.
A. Typical Service Life Ranges
Values below are example ranges and may vary widely by line conditions.
| Grade | Industry/Process | Continuous Use Before Replacement | Regrind Interval (Meters/Strokes) | Regrind Cycles | Notes |
| WC–Co | Film/foil slitting | 80–200 h | 200–600 km | 5–10× | Filled/fiber materials reduce life |
| WC–Co | Granulator & recycling | 40–120 h | N/A | 3–6× | Strongly affected by impact/foreign objects |
| SKH51 | Film/paper slitting | 20–60 h | 60–200 km | 3–6× | Coating improves life; thermal control is critical |
| SKD11 | Metal shearing/punching | 24–72 h | 50–200k strokes | 3–5× | Cryo improves stability |
| SKD11 | Rubber/tire cutting | 30–90 h | 10–40 km | 3–6× | Friction/heat/contamination strongly affect life |
| SUS440C | Food/wet lines/frequent cleaning | 40–120 h | 30–120 km | 2–4× | Highly dependent on corrosion/cleaning conditions |
| 420J2 | Food slicing/packaging (low load) | 40–120 h | 30–120 km | 2–4× | Economical; lower hardness |
| SK5 | Paper/low-difficulty cutting | 10–40 h | 10–60 km | 1–3× | Low cost, faster wear |
Note: S45C/SCM440 are structural/holder materials rather than cutting-edge grades, so they are excluded from blade life tables.
B. Life Multipliers
| Factor | Condition | Multiplier |
| Coating | TiN/TiAlN (dry/high speed) | ×1.2–×1.4 |
| DLC (anti-stick/cleanliness) | ×1.1–×1.3 |
| Work material | Filled/glass-fiber/carbon-filled | ×0.5–×0.7 |
| Line speed | +20% vs baseline | ×0.85–×0.95 |
| Gap/angle optimization | Precision setup maintained | ×1.1–×1.3 |
| Lubrication/cooling | Properly maintained | ×1.05–×1.2 |
| Contamination/misalignment | Chips/stickiness/eccentricity | ×0.6–×0.9 |
Limitation: These multipliers provide conservative estimates using a simplified model. In real production, nonlinear interactions between variables may occur.
1. Materials at a Glance
A. Material Summary
This is a quick reference to help operators choose the right material efficiently.
Covered grades: WC, SKH51, SKD11, SUS440C, 420J2, SK5, S45C (AISI 1045), SCM440 (AISI 4140)
* SK5 target hardness can vary depending on geometry, quench method (oil/water), and distortion control.
Note: S45C/SCM440 are recommended for holders/fixtures/structural parts rather than cutting edges.
B. Key Trade-off: Hardness (HRC) vs Toughness
Understanding the trade-off between wear resistance and impact resistance (toughness) helps you select the right grade.
C. Typical Chemistry (wt%)
The ranges below are typical values. Actual chemistry should follow the applicable standard, supplier specification, and mill test certificate (MTC).
2. Heat Treatment & Coating
A. Recommended Heat-Treat Summary
The following are general guidelines. Actual parameters should be adjusted based on section thickness, geometry, equipment (vacuum/gas/salt/oil), and target microstructure.
Soak time is shown as “after equalization” (when the entire section has reached the target temperature).
440C tempering note (corrosion resistance):
To maintain corrosion resistance, low-temperature tempering at 150–200°C is recommended. In general, the ~425–565°C range has a higher risk of corrosion resistance loss (sensitization/carbide precipitation), so it is safer to avoid unless specifically required.
B. Coating Selection Guide
3. Specs & Tolerances
A. Standard Dimensions
A-1. Circular Slitter
A-2. Straight / Shear Blade
B. Tolerance Classes
Balancing note (ISO 21940): G2.5 is advantageous for vibration control on high-speed/precision lines, but the required grade depends on speed, holder design, and assembly condition.
C. Surface & Edge Finish
4. Reference Conditions & Performance Modeling
Disclaimer: This document is an engineering guideline provided by HD KNIFE and should not be treated as guaranteed performance. Actual tool life varies significantly depending on line conditions (gap, speed, lubrication, material, setup accuracy, foreign objects, etc.). Sample evaluation is recommended for first-time applications.
A. Typical Service Life Ranges
Values below are example ranges and may vary widely by line conditions.
Note: S45C/SCM440 are structural/holder materials rather than cutting-edge grades, so they are excluded from blade life tables.
B. Life Multipliers
Limitation: These multipliers provide conservative estimates using a simplified model. In real production, nonlinear interactions between variables may occur.